The Measures And Effects Of Nitrogen Increase In High Nitrogen Stainless Steel Melting

Publish Time: Author: Site Editor Visit: 35195

The Measures And Effects Of Nitrogen Increase In High Nitrogen Stainless Steel Melting

High-nitrogen stainless steel refers to a steel with a ferrite matrix with a nitrogen content of more than 0.08% (mass fraction, the same below) or an austenite matrix with a nitrogen content of more than 0.4%. High nitrogen stainless steel has many advantages, such as high strength and toughness, good ductility, low magnetic permeability, and good corrosion resistance.

These characteristics are mainly due to the addition of nitrogen. In the early stage, if nitrogen residues appeared in the steel, it would cause age hardening, pores and segregation, resulting in defects or even scrapping of steel castings.

Later, researchers found that nitrogen can significantly increase the strength of steel, increase the stability of the austenite structure in steel, and improve the pitting and crevice corrosion resistance of steel.

In order to study the nitrogen-increasing effect of nitrogen injection and addition of chromium-nitride alloy on molten steel, the scholars smelted high-nitrogen nickel-free stainless steel (17Cr12Mn2Mo) by changing the nitrogen partial pressure, temperature and adding chromium-nitride alloy on a 50kg vacuum induction melting furnace. And compare the test results with the theoretical calculation results.

Experiments show that by changing the nitrogen partial pressure and temperature, stainless steel with a certain nitrogen content can be smelted. The nitrogen increase effect of increasing the nitrogen partial pressure is more obvious than changing the temperature. When the nitrogen partial pressure reaches 0.65MPa, the measured nitrogen content can reach the theoretical value; Adding a nitrogen-containing alloy to smelt high-nitrogen stainless steel has a greater nitrogen-increasing effect than adjusting temperature and nitrogen partial pressure, and the actual nitrogen content is higher than the theoretical value.


Please keep the source and address of this article for reprinting: The Measures And Effects Of Nitrogen Increase In High Nitrogen Stainless Steel Melting


Minghe Die Casting Company are dedicated to manufacture and provide quality and high performance Casting Parts(metal die casting parts range mainly include Thin-Wall Die Casting,Hot Chamber Die Casting,Cold Chamber Die Casting),Round Service(Die Casting Service,Cnc Machining,Mold Making,Surface Treatment).Any custom Aluminum die casting, magnesium or Zamak/zinc die casting and other castings requirements are welcome to contact us.

ISO90012015 AND ITAF 16949 CASTING COMPANY SHOP

Under the control of ISO9001 and TS 16949,All processes are carried out through hundreds of advanced die casting machines, 5-axis machines, and other facilities, ranging from blasters to Ultra Sonic washing machines.Minghe not only has advanced equipment but also have professional team of experienced engineers,operators and inspectors to make the customer’s design come true.

POWERFUL ALUMINUM DIE CASTING WITH ISO90012015

Contract manufacturer of die castings. Capabilities include cold chamber aluminum die casting parts from 0.15 lbs. to 6 lbs., quick change set up, and machining. Value-added services include polishing, vibrating, deburring, shot blasting, painting, plating, coating, assembly, and tooling. Materials worked with include alloys such as 360, 380, 383, and 413.

PERFECT ZINC DIE CASTING PARTS IN CHINA

Zinc die casting design assistance/concurrent engineering services. Custom manufacturer of precision zinc die castings. Miniature castings, high pressure die castings, multi-slide mold castings, conventional mold castings, unit die and independent die castings and cavity sealed castings can be manufactured. Castings can be manufactured in lengths and widths up to 24 in. in +/-0.0005 in. tolerance.  

ISO 9001 2015 certified manufacturer of die cast magnesium and mold manufacturing

ISO 9001: 2015 certified manufacturer of die cast magnesium, Capabilities include high-pressure magnesium die casting up to 200 ton hot chamber & 3000 ton cold chamber, tooling design, polishing, molding, machining, powder & liquid painting, full QA with CMM capabilities, assembly, packaging & delivery.

Minghe Casting Additional Casting Service-investment casting etc

ITAF16949 certified. Additional Casting Service Include investment casting,sand casting,Gravity Casting, Lost Foam Casting,Centrifugal Casting,Vacuum Casting,Permanent Mold Casting,.Capabilities include EDI, engineering assistance, solid modeling and secondary processing.

Casting Parts Application Case Studies

Casting Industries Parts Case Studies for: Cars, Bikes, Aircraft, Musical instruments, Watercraft, Optical devices, Sensors, Models, Electronic devices, Enclosures, Clocks, Machinery, Engines, Furniture, Jewelry, Jigs, Telecom, Lighting, Medical devices, Photographic devices, Robots, Sculptures, Sound equipment, Sporting equipment, Tooling, Toys and more. 


What Can we help you do next?

∇ Go To Homepage For Die Casting China

→Casting Parts-Find out what we have done.

→Ralated Tips About Die Casting Services


By Minghe Die Casting Manufacturer |Categories: Helpful Articles |Material Tags: , , , , , ,Bronze Casting,Casting Video,Company History,Aluminum Die Casting |Comments Off

MingHe Casting Advantage

  • Comprehensive Casting design software and skilled engineer enables sample to be done within 15-25 days
  • Complete set of inspection equipment & quality control makes excellent Die Casting products
  • A fine shipping process and good supplier guarantee we can always deliver Die Casting goods on time
  • From prototypes to end parts, upload your CAD files, fast and professional quote in 1-24 hours
  • Wide-ranging capabilities for designing prototypes or massive manufacturing end use Die Casting parts
  • Advanced Die Casting techniques (180-3000T Machine,Cnc Machining, CMM) process a variety of metal & plastic materials

HelpFul Articles

The Introduction To Automobile Lightweight Process

At present, with the adjustment of energy structure and the improvement of environmental protection

Machining Performance Comparison Between CNC And RP

In the past fifteen years, significant progress has been made in prototype replication. Initially, m

The Influence Of Three Cutting Elements On Machining Efficiency

Everyone knows that when improving machining efficiency, increasing the three elements of cutting (c

Comprehensive Diagnosis And Control Of Automobile Aluminum Die Castings Quality

With the continuous development of sports and science and technology, people's living standards cont

The Maintenance Of Automobile Molds

The first-level maintenance of the mold refers to the operation and daily maintenance of the mold du

Daily Maintenance And Molds Safety Protection

As the most important production tool of a die-casting factory, it determines the shape, specificati

Mould Heat Treatment Surface Strengthening And Modification Technology

Mold shot peening and action shot peening process is the process of ejecting a large number of proje

The Calculation Method Of Mold Making Price

Empirical calculation method mold price = material cost + design cost + processing cost and profit +

The Reasons For Aluminum Die Casting Tooling Easy Cracking

As we all know, aluminum alloy die steel die-casting die will have cracks after a period of producti

The Key Points For The Production And Aluminum Alloy Die-Casting Molds Use

Aluminum alloy die-casting molds have high technical requirements and high cost, which is one of the

The Measures To Improve The Life Of Aluminum-Magnesium Alloy Die Casting Mold

As an important processing equipment, aluminum-magnesium alloy die-casting molds have a direct impac

The Advantages And Disadvantages Of Aluminum Casting Process

Due to the different elements of each group of aluminum alloys, the physical and chemical properties

What Is Pressure Die Casting? What Is Die-Casting Process?

High pressure casting is a kind of special casting method with less cutting and no cutting which has

Die Casting- A Typical Digital Industry Case Sharing

Die casting, also known as high pressure casting, is a near net shape technology that has been widel

Four Non-Specific Surface Treatments Of Aluminum Alloy Die Castings

In actual production, many aluminum alloy casting enterprises will encounter the confusion of the ug

Recycled Aluminum Processing Production Technology And Development Direction

The reuse of resources is an important means of building an "environmentally friendly, green" produc

Seven Problems And Solutions Of Surface Casting Defects

The surface of the casting is line-shaped strain along the mold opening direction, with a certain de

Seven Precautions In Drawing Die Design

Stretching dies account for a very large proportion of the entire stamping die industry. Our common

Methods And Steps Of Stamping Die Design

There are many types of molds, which can be divided into: ①Metal molds based on processing goals and

The Problems and Solutions of Internal Defects of Aluminum Alloy Die Castings

The appearance inspection or metallographic inspection during mechanical processing or after CNC mac